Most machined aluminum parts are made from one of two alloys. 6061-T6 is the general-purpose choice: easy to machine, weldable, corrosion resistant, and widely stocked. 7075-T6 is the high-strength choice, with close to twice the yield strength, at a higher material cost and with real trade-offs in welding and corrosion. Picking between 6061 vs. 7075 comes down to load, environment, and what happens to the part after machining.

Strength

This is the main reason to specify 7075. Typical published values for the T6 temper:

Property (typical, T6) 6061-T6 7075-T6
Ultimate tensile strength 45 ksi (310 MPa) 83 ksi (572 MPa)
Yield strength 40 ksi (276 MPa) 73 ksi (503 MPa)
Density 0.098 lb/in³ (2.70 g/cm³) 0.102 lb/in³ (2.81 g/cm³)
Weldability Good Poor (generally not fusion welded)
General corrosion resistance Good Fair

Values are typical published figures and vary by product form and thickness. Check the material spec for design values.

For a bracket, fixture, or housing with modest loads, 6061 has more than enough strength. For highly stressed structural parts, thin sections that have to carry load, or parts where weight savings depend on a smaller cross-section, 7075 earns its price. That is why it shows up so often on aerospace and defense drawings.

Welding

6061 welds well with TIG or MIG, though the heat-affected zone loses strength unless the part is re-heat-treated. 7075 is generally considered unsuitable for fusion welding because it is prone to cracking. If your part belongs to a welded assembly, 6061 is almost always the answer.

Corrosion

6061 holds up well in most environments. 7075 has lower general corrosion resistance, and in the T6 temper it is susceptible to stress corrosion cracking under sustained tensile stress. The T73 temper trades some strength for much better stress corrosion resistance, which is why you will see 7075-T73 or T7351 called out on some aerospace parts. Either alloy is usually anodized or coated in harsh environments. Our corrosion resistant alloys guide compares aluminum with stainless and nickel alloys.

Machining

Both alloys machine well. 7075 is harder and tends to produce cleaner chips and finer surface finishes, especially on thin walls and small features. 6061 can be slightly gummier, but it is forgiving and fast. In practice, machining time is rarely the deciding factor. Material cost and availability matter more: 6061 bar and plate are stocked everywhere in most sizes, while some 7075 sizes and tempers take longer to source.

Anodizing and finishing

6061 anodizes evenly and is the usual choice for cosmetic parts with clear or dyed finishes. 7075 also anodizes well, though Type III hard anodize can come out darker, and color matching across the two alloys is difficult. If parts made from both alloys need to look the same in an assembly, say so on the drawing. See finishing and post-processing for options.

How to choose

  • Choose 6061-T6 for general parts, welded assemblies, cosmetic anodized parts, and anything where cost and availability matter more than peak strength.
  • Choose 7075-T6 for highly loaded structural parts, thin load-bearing sections, and weight-critical designs where 6061 would need a larger cross-section.
  • Consider 7075-T73 or T7351 when a high-strength part will see sustained stress in a corrosive environment.
  • If strength-to-weight still isn’t enough, compare against titanium. Our aluminum vs. titanium guide covers that decision.

Machining aluminum with PE

PE places aluminum work across a vetted network of CNC machining shops, from quick-turn prototypes to production lots, with material certs and inspection before parts ship. If you’re unsure which alloy fits, send the drawing and we’ll review it before we quote. We support aerospace, defense, and commercial products programs.

Frequently asked questions

Yes. In the T6 temper, 7075 has roughly 83 ksi ultimate tensile strength and 73 ksi yield, compared with about 45 ksi and 40 ksi for 6061-T6.

7075 is generally not fusion welded because it is prone to cracking. Use 6061 for welded assemblies, or join 7075 parts mechanically.

6061 has better general corrosion resistance. 7075-T6 is also susceptible to stress corrosion cracking, which the T73 temper improves.

6061 usually costs less overall because the material is cheaper and widely stocked. Machining time between the two is similar.